Skip to content
Welcome to ATM-Magnet
Application Notes

Magnet industry insights, product updates and application notes from ATM-Magnet.

Coating Options for Corrosion-Resistant Magnets

Published:2026-09-11    Category:Application Notes    Views:10

Coating Options for Corrosion-Resistant Magnets

Sintered neodymium magnets corrode readily, and they corrode in a way that is worse than ordinary rust. Because their microstructure contains a reactive neodymium-rich phase between the magnetic grains, moisture attacks preferentially along the grain boundaries, and the material can lose structural integrity and shed a fine powder rather than simply staining. A coating is therefore not a cosmetic finish on a magnet — it is a functional barrier that determines whether the component survives its service environment.

Choosing that barrier is a trade between corrosion performance, coating thickness, temperature capability, electrical behaviour and cost. This guide sets out the options and the reasoning behind each.

Why Neodymium Magnets Corrode So Readily

A sintered NdFeB magnet is not a single homogeneous material. It is a dense array of Nd&sub2;Fe&sub1;₄B grains bonded by a thin neodymium-rich boundary phase. The magnetic properties come from the grains; the boundary phase is electrochemically active and far less noble than the interior. In the presence of moisture and oxygen, this boundary phase becomes the preferred corrosion path, and the attack is intergranular.

Three consequences follow directly:

  • Corrosion starts at exposed surfaces and edges, and propagates inward along grain boundaries rather than staying on the surface.
  • Because the boundary phase is also a weakness in fracture terms, corroded magnets become brittle and prone to chipping and pulverization.
  • Any coating defect — a pinhole, a thin corner, a handling scratch — creates a locally concentrated attack site, so coating quality at edges matters more than average thickness.

The grade itself also plays a part. Higher-coercivity classes that contain more dysprosium or terbium, and grades with cobalt additions, typically resist corrosion somewhat better than basic high-remanence grades, but the difference is a secondary effect. The coating remains the primary protection.

What a Coating Has to Achieve

Requirement Why it matters
Barrier against moisture and oxygen Prevents the intergranular attack that destroys the magnet
Complete edge and corner coverage Edges are where corrosion and chipping begin
Adhesion to a brittle substrate Poor adhesion leads to flaking under thermal cycling and handling
Thermal compatibility Must survive both the application process temperature and the service temperature
Controlled thickness Coating adds to all surfaces and changes critical dimensions
Electrical behaviour Segment insulation requires a non-conductive coating; conductive contact requires the opposite

The Main Coating Options

Coating Typical thickness Commonly reported salt spray Appearance Relative cost
Nickel-copper-nickel Approx. 10–25 µm total Approx. 24–96 hours, higher with optimized plating Bright metallic silver Baseline
Zinc Approx. 4–15 µm Approx. 24–72 hours, higher at greater thickness Blue-white to dull grey Low
Epoxy Approx. 10–30 µm Approx. 200–1,000 hours depending on system Matte, colour options Low to moderate
Aluminium-based Approx. 10–30 µm Approx. 100–500 hours Bright silver Moderate
Zinc-aluminium (flake) Approx. 5–15 µm Commonly above 500 hours Matte silver to grey Moderate
Parylene Approx. 5–25 µm Hundreds of hours Clear, transparent High
PTFE Approx. 10–30 µm Chemically inert; moderate salinity protection Dark, low friction High
Nickel-chromium duplex Approx. 10–30 µm Among the best of the metallic systems Bright, slightly blue-white Moderate to high
Phosphate Approx. 1–5 µm Limited on its own Dark grey, matte Low
Tin Approx. 5–15 µm Moderate Bright silver-white Low to moderate
Gold Approx. 1–5 µm Very high Gold, conductive Very high

Salt spray figures quoted by different suppliers are not directly comparable. A number means nothing without the coating thickness, the test standard, the concentration, the chamber temperature and the pass criteria that were used. Two suppliers reporting “48 hours” may be describing very different performance. Specify the thickness and the standard, and require the test report rather than the headline number.

Nickel-Copper-Nickel: The Default Choice

Nickel-copper-nickel is the most widely used magnet coating and the sensible starting point for most applications. The three-layer structure exists for a reason. The first nickel layer bonds to the magnet surface; the copper interlayer is ductile and compliant, which absorbs thermal expansion mismatch and stops cracks propagating through to the substrate; the outer nickel layer provides hardness and wear resistance.

Its strengths are a good cost-to-performance ratio, a durable surface that resists handling damage, and conductivity where electrical contact is required. Its limitations are equally clear. Being conductive, it cannot insulate segments from each other in a motor magnet assembly where eddy-current suppression depends on electrical isolation. Salt spray performance is adequate for indoor and moderate outdoor use but falls short of what epoxy or aluminium-based systems achieve. It also throws less evenly into recesses and blind features than a chemically deposited coating would.

Zinc Coatings

Zinc is the economical option. It protects partly by acting as a sacrificial anode, which means it keeps protecting the magnet even where the coating is locally damaged — an advantage that barrier coatings do not offer. Blue-white and clear passivations are common, and thicker deposits extend the salt spray time considerably.

The trade-offs are lower temperature capability and a thinner, softer film that is easier to damage during handling and assembly. For indoor products, low-cost assemblies, or where the environment is genuinely benign, zinc is often the most rational choice. For hot or aggressive service it is usually the wrong one.

Epoxy Coatings

Epoxy is the strongest performer among the low-cost options for salt spray resistance, and it has the useful property of being electrically insulating. That combination makes it the natural choice for motor and generator magnets, and for any segmented assembly where the layers between segments must both protect and insulate. It also accepts colour, which matters for consumer-facing products.

Two constraints govern its use. The first is temperature: epoxy systems are limited by the thermal capability of the resin, so the cure schedule and the service temperature both have to be checked against the magnet’s application. The second is mechanical: epoxy is more susceptible to edge chipping than a metallic coating during handling, so packaging and assembly handling need to be controlled.

Aluminium-Based Coatings

Aluminium coatings applied by ion vapour deposition or physical vapour deposition offer a combination that few other systems match: good corrosion resistance from a relatively thin, dense and pore-free film, high temperature capability, and no risk of the coating interfering with magnetic performance. They are frequently selected for motors, actuators and sensors where the magnet sees sustained heat.

The process requires vacuum equipment, so it carries a cost and lead time penalty compared with electroplating and is available from a smaller supplier base. Film thickness control and surface cleanliness are critical because the coating is deposited rather than chemically bonded.

Specialty Barrier Coatings

Three coatings address environments that the mainstream options handle poorly:

Coating Distinguishing property Where it earns its cost
Parylene Deposited from vapour, so it coats every exposed surface uniformly, including edges and complex geometry Small precision parts, medical devices, sensors where pinholes are unacceptable
PTFE Chemically inert and low friction Exposure to acids, solvents and fuels; sliding or release applications
Molybdenum disulphide based systems Combined corrosion and chemical resistance with a low-friction surface Severe combined chemical and corrosion environments

Conductive and Precious Metal Coatings

Where the magnet must make electrical contact or be soldered, gold, silver and tin coatings are used. Gold gives the best combination of corrosion resistance and stable contact resistance, at a cost that limits it to small, high-value components. Silver has excellent conductivity but tarnishes. Tin is inexpensive and solderable but offers only moderate corrosion protection.

Nickel-chromium duplex coatings are worth noting separately. A nickel undercoat with a chromium topcoat has been shown in published corrosion studies to be among the most effective of the metallic systems tested, with a hard, bright surface. The additional process step and cost mean it is normally reserved for applications where the extra performance is genuinely required.

Selection by Environment

Service condition Reasonable choice Reason
Indoor, dry, benign Zinc or thin nickel-copper-nickel Cost is the governing factor
General outdoor, humid Epoxy or zinc-aluminium Substantially better salt spray than plated nickel
Motor or generator rotor Epoxy, or aluminium-based at high temperature Insulation plus protection, with thermal headroom
Sustained heat above 150 °C Aluminium-based Remains effective where resin coatings degrade
Marine or chloride exposure Epoxy or aluminium-based, with sealed edges Plated nickel alone is usually insufficient
Acids, solvents or fuels PTFE or molybdenum disulphide systems Chemical inertness, not just water resistance
Medical, implant or hygienic Parylene or gold Pinhole-free coverage and cleanable surfaces
Segmented magnet assemblies Epoxy or other insulating systems Conductive coatings short the segments together
Soldered or electrically contacted Tin, silver or gold, often over a nickel base Solderability and stable contact resistance

Thickness and Dimensional Consequences

Every applied coating increases the size of the magnet on every coated surface. That effect is easy to overlook because the thicknesses involved are small, but magnets are frequently specified to tight tolerances and the coating can consume a meaningful part of the allowance.

Coating Growth per coated surface Planning note
Nickel-copper-nickel Roughly 5–12 µm Coat after grinding; account for it on mating faces
Zinc Roughly 2–8 µm Smallest dimensional effect of the common coatings
Epoxy Roughly 5–15 µm Significant on thin magnets; can be locally masked
Aluminium-based Roughly 5–15 µm Compare against air-gap allowance in the magnetic design
Parylene Roughly 3–12 µm Very uniform, including edges and recesses
Gold Roughly 0.5–2.5 µm Often applied over a nickel strike layer

The coating must always be applied after the final grinding or machining operation. Coating a magnet and then grinding it destroys the barrier exactly where it is most needed. Where a face must remain conductive or dimensionally exact, that face is masked before coating, and masking has to be defined on the drawing rather than agreed verbally.

Process Temperature and Magnet Compatibility

The temperature a coating process reaches is a real constraint, though less often than for other components, because the magnet’s own service limit is usually lower. Electroplated and electroless processes run near ambient and pose no thermal risk. Epoxy cure temperatures need checking against the resin and the magnet’s application. Vacuum-deposited aluminium and precious metal coatings are applied at elevated temperature but are used precisely because the application itself is hot.

The more common issue is the opposite one: a coating chosen for cost that cannot survive the service temperature. A zinc or standard epoxy film on a magnet that operates near 150 °C will degrade long before the magnet does, and the resulting failure looks like a corrosion problem when it is really a thermal-selection problem.

Test Standards and How to Read a Claim

Property Standard or method
Neutral salt spray ASTM B117, ISO 9227
Humidity and pressure cooker exposure Accelerated humidity or HAST method agreed with the customer
Coating adhesion ASTM D3359 or equivalent cross-hatch method
Coating thickness X-ray fluorescence or cross-section measurement
Zinc plating specification ASTM B633 or the customer’s own plating specification
Magnetic performance after coating Flux or magnetic moment measurement before and after coating

The last row is worth emphasising. A coating should not change magnetic output, but the test confirms it, and it also catches process problems such as excessive heat or surface damage during preparation. Where a magnet is machined to final size before coating, this check closes the loop between dimensions, coating and magnetic result.

Failure Modes to Watch

  • Edge corrosion. Coverage thins at sharp corners in electroplated systems, and that is where corrosion begins. Chamfering or controlled edge radius helps.
  • Coating flaking under thermal cycling, usually from adhesion problems or mismatched expansion rather than from the coating chemistry itself.
  • Galvanic attack where the coating contacts a more noble metal in the presence of moisture, which can accelerate coating loss.
  • Shorting in segmented assemblies where a conductive coating was specified by habit rather than by requirement.
  • Corrosion that starts at a handling scratch, which is a packaging and assembly-control issue rather than a coating-selection issue.
  • Degradation of the coating at temperature while the magnet itself is still within its own operating limits.

A Practical Selection Sequence

  1. Define the actual environment: humidity, salt, chemicals, condensing conditions and the time spent at each.
  2. Establish the maximum service temperature of the magnet in the application, including transient excursions.
  3. Decide whether the coating must insulate or conduct, since this eliminates half the options immediately.
  4. Set the dimensional allowance available, and check that the coating thickness fits within it.
  5. Choose the coating family on the basis of environment and temperature, then select a specific system by cost.
  6. Confirm the coating is compatible with the magnet grade, particularly where high-coercivity grades or cobalt-containing grades are used.
  7. Specify thickness and test standard, and require test reports rather than accepting a salt spray headline.
  8. Define masked areas, edge treatment and packaging requirements explicitly on the drawing.
  9. Validate with salt spray, adhesion and magnetic-performance checks on the production process, not only on samples.

About ATM-Magnet

ATM-Magnet supplies sintered neodymium magnets with coating options covering nickel-copper-nickel, zinc, epoxy, aluminium-based, zinc-aluminium, Parylene, PTFE, tin and precious metal systems, matched to the corrosion, temperature and electrical requirements of the application. Coating selection is handled together with grade, geometry and tolerance decisions, since thickness allowance, insulation requirements and service temperature all interact. Thickness measurement, adhesion and salt spray testing are available against recognized standards, together with magnetic performance verification before and after coating.

Chat

Chat Pre-sales Agent

Chat After-sales Agent

Chat

Request Callback

24h Callback Service

Enter your phone number and area code

Request Callback

WeChat Scan to Visit

WeChat QR Code

WeChat
Back to Top